Page 213
... impact tests , we cut the ice sheet into free - floating , octagonal shaped ice floes and impact them with moving sheet pile mounted under the carriage . For tests with change in water level , we freed a large ice sheet from the basin ...
... impact tests , we cut the ice sheet into free - floating , octagonal shaped ice floes and impact them with moving sheet pile mounted under the carriage . For tests with change in water level , we freed a large ice sheet from the basin ...
Page 242
... impact transition curves are shown in Figure 5 ( 12 ) for ABS - B plate . These data highlight particularly the effect of orientation on Charpy impact behaviour for steels in the as - rolled condition , values at 0 ° C for transverse ...
... impact transition curves are shown in Figure 5 ( 12 ) for ABS - B plate . These data highlight particularly the effect of orientation on Charpy impact behaviour for steels in the as - rolled condition , values at 0 ° C for transverse ...
Page 259
... impact properties Strain and Charpy impact properties Location Direction aging " Absorbed energy ( J ) 50 % -60 ° C -80 ° C -100 °C | FATT ( C ) -10-20-3040-50 -60 Fig.8 Results of temperature gradient type of ESSO. Tensile properties ...
... impact properties Strain and Charpy impact properties Location Direction aging " Absorbed energy ( J ) 50 % -60 ° C -80 ° C -100 °C | FATT ( C ) -10-20-3040-50 -60 Fig.8 Results of temperature gradient type of ESSO. Tensile properties ...
Contents
STRUCTURAL INTEGRITY PROCEDURES FOR EUROPE SINTAP | 1 |
OMAE99MAT2041 | 9 |
Development of the SINTAP Failure Assessment Diagrams for Compatibility With | 19 |
Copyright | |
28 other sections not shown
Other editions - View all
Common terms and phrases
addition analysis applications approach ASME assessment base behavior bending CGHAZ Charpy compared component composite condition Conference Copyright crack critical CTOD curve defects deposition depth determined developed distribution dynamic effect element energy Engineering equations equivalent evaluated factors failure fatigue ferrite Figure fire fracture toughness function geometry given hardness heat input impact important improve increase initiation International joints length limit loading lower material matrix maximum mean measured mechanical method microstructure molten observed obtained offshore operating parameters performance phase pipe plate prediction present pressure procedure production properties protection range ratio reduced region requirements residual stress respectively risers safety ship shown shows specimens standards steel strain strength structures surface Table temperature tensile thickness values weld metal welded joints wire yield